Properties
| Measurement |
Test Method |
Value (90 minute UV post-cured) |
Value (90 minute UV + 2 hours @ 80ºC thermal post-cured) |
| Hardness, Shore D |
ASTM D 2240 |
79 |
81 |
Flexural Modulus
Flexural Strength |
ASTM D 790 |
1,390-1,560 Mpa (200-225 KSI)
50-55 Mpa (7,300-8,000 PSI) |
1,460-1,600 Mpa (210-230 KSI)
52-56 Mpa (7,500-8,100 PSI) |
Tensile Modulus
Tensile Strength
Elongation at Break |
ASTM D 638 |
1,400-1,900 Mpa (200-275 KSI)
35-40 Mpa (5,000-5,700 PSI)
12-21% |
1,500-1,900 Mpa (220-280 KSI)
35-40 Mpa (5,000-5,700)
10-16% |
| Impact Strength, Notched Izod |
ASTM D 256 |
28-39 J/m (0.5-0.7 ft-lbs/in) |
22-33 J/m (0.4-0.6 ft-lbs/in) |
| Heat Deflection Temperature |
ASTM D 648 @66 PSI ASTM D 648@264 PSI |
48-50ºC (118-122ºF)
43-48ºC (109-118ºF) | 58-60ºC (136-140ºF) 48-50ºC (118-122ºF) |
| Glass Transition (Tg) |
DMA, E" peak |
55ºC (131ºF) |
58ºC (136ºF) |
| Density |
|
1.19 g/cm3 |
|